17-4 PH
Also known as UNS S17400, EN 1.4542
17-4 PH (also written 17-4PH, Type 630 or AISI 630; UNS S17400, EN 1.4542) is a martensitic precipitation-hardening stainless steel offering high strength with corrosion resistance similar to 304.
Key facts
- Type
- Martensitic precipitation-hardening stainless steel
- UNS / EN
- UNS S17400 / EN 1.4542 (X5CrNiCuNb16-4)
- Also designated
- Type 630, AISI 630, 17-4PH, ASTM A564 Type 630, AMS 5643
- Density
- 7.75 g/cm³ (7750 kg/m³)
- 0.2% proof stress
- 380-1170 N/mm² by condition
- Tensile strength
- 860-1310 N/mm² by condition
- Strength retained to
- 316°C (600°F)
- Magnetic
- Yes (ferromagnetic)
- Corrosion resistance
- Comparable to Alloy 304
- Forms
- Bar stocked; plate, tube and fittings on enquiry; forgings and castings to order
- Stocked conditions
- Condition A and H1150D from stock; H900 to H1150 aged to order
- Sour service
- NACE MR0175 / ISO 15156-3 in the double-aged H1150D condition, within its hardness limit
17-4 PH (UNS S17400), often written 17-4PH, is a martensitic precipitation hardening stainless steel, also sold as Type 630 or AISI 630 and, in Europe, as EN 1.4542. Its main alloying elements are chromium (17%) and nickel (4%), with significant copper additions (typically 4%) that form highly dispersed precipitate particles on ageing, the mechanism that delivers high strength.
Eight heat-treatment conditions provide a wide range of strength and toughness combinations. In Condition A (solution annealed) the grade is in its most machinable state; subsequent ageing at temperatures from 482°C (H900) to 760°C (H1150D) develops the required mechanical properties. Higher ageing temperatures produce lower strength but improved toughness and corrosion resistance.
How the conditions work. After solution treatment and a water quench, ageing at a controlled temperature precipitates fine copper-niobium particles that harden the martensite. The number in each name is the ageing temperature in °F, so H900 is aged at 482°C (900°F) for 1 hour and gives the highest strength (1170 N/mm² 0.2% proof stress), while H1150 is aged at 621°C (1150°F) for 4 hours. Hotter ageing lets the precipitates coarsen, so strength falls and toughness rises. H1150D is double aged: 760°C (1400°F) for 2 hours, air cooled, then 621°C for 4 hours, which gives the best toughness of the listed conditions (75 J impact strength). See our guide to what precipitation hardening is for the wider mechanism.
Martensitic stainless steels retain their strength and toughness at temperatures up to 316°C (600°F), supporting use in oil and gas and chemical processing applications. Because 17-4 PH is martensitic it is magnetic; our article on austenitic and martensitic stainless steel explains the difference, and which stainless steels are non-magnetic.
Bar is stocked in Condition A and H1150D; the other aged tempers are aged to order. Plate, tube and fittings are available on enquiry; forgings and castings to order. Download the 17-4 PH datasheet (PDF) (opens in new tab) for composition, mechanical properties in all eight conditions and machining guidance.
17-4 PH is part of our stainless steel range. Where corrosion resistance matters more than strength, Alloy 316L is the usual alternative, and Fermonic® 50 is a high-strength austenitic option. The designations are cross-referenced in our standards guide, and for sour service see what NACE MR0175 requires.
- Higher strength than most other stainless steels through precipitation hardening
- Corrosion resistance acceptable for many corrosive environments
- Good resistance to wear
- Retains strength and toughness at temperatures up to 316°C (600°F)
- Annealed condition (Condition A) allows easy machining before final age hardening
- Eight defined conditions allow properties to be tailored precisely to the application
| Element | Min | Max |
|---|---|---|
| Iron (Fe) | Bal | |
| Chromium (Cr) | 15.00 | 17.50 |
| Nickel (Ni) | 3.00 | 5.00 |
| Copper (Cu) | 3.00 | 5.00 |
| Niobium+Tantalum (Nb+Ta) | 0.15 | 0.45 |
| Manganese (Mn) | - | 1.00 |
| Carbon (C) | - | 0.07 |
| Silicon (Si) | - | 1.00 |
| Phosphorus (P) | - | 0.04 |
| Sulphur (S) | - | 0.01 |
| Property | Imperial | Metric |
|---|---|---|
| 0.2% Proof stress (min) | 55 ksi | 380 N/mm² |
| Tensile strength | 175 ksi | 1200 N/mm² |
| Elongation (5.65√S0 & 4D) | 35% | |
| Reduction of area | 55% | |
| Hardness (Brinell) | 363 max | |
| Impact strength (room temp) | 40 ft.lb | 54 J |
| Property | Imperial | Metric |
|---|---|---|
| 0.2% Proof stress (min) | 170 ksi | 1170 N/mm² |
| Tensile strength (min) | 190 ksi | 1310 N/mm² |
| Elongation (5.65√S0 & 4D) | 10% | |
| Reduction of area | 40% | |
| Hardness (Brinell) | 388 min |
| Property | Imperial | Metric |
|---|---|---|
| 0.2% Proof stress (min) | 155 ksi | 1070 N/mm² |
| Tensile strength (min) | 170 ksi | 1170 N/mm² |
| Elongation (5.65√S0 & 4D) | 10% | |
| Reduction of area | 44% | |
| Hardness (Brinell) | 375 min | |
| Impact strength (room temp) | 5 ft.lb | 7 J |
| Property | Imperial | Metric |
|---|---|---|
| 0.2% Proof stress (min) | 145 ksi | 1000 N/mm² |
| Tensile strength (min) | 155 ksi | 1070 N/mm² |
| Elongation (5.65√S0 & 4D) | 12% | |
| Reduction of area | 45% | |
| Hardness (Brinell) | 331 min | |
| Impact strength (room temp) | 15 ft.lb | 20 J |
| Property | Imperial | Metric |
|---|---|---|
| 0.2% Proof stress (min) | 125 ksi | 860 N/mm² |
| Tensile strength (min) | 145 ksi | 1000 N/mm² |
| Elongation (5.65√S0 & 4D) | 13% | |
| Reduction of area | 45% | |
| Hardness (Brinell) | 311 min | |
| Impact strength (room temp) | 20 ft.lb | 27 J |
| Property | Imperial | Metric |
|---|---|---|
| 0.2% Proof stress (min) | 115 ksi | 795 N/mm² |
| Tensile strength (min) | 140 ksi | 965 N/mm² |
| Elongation (5.65√S0 & 4D) | 14% | |
| Reduction of area | 45% | |
| Hardness (Brinell) | 302 min | |
| Impact strength (room temp) | 25 ft.lb | 34 J |
| Property | Imperial | Metric |
|---|---|---|
| 0.2% Proof stress (min) | 105.1 ksi | 725 N/mm² |
| Tensile strength (min) | 134.8 ksi | 930 N/mm² |
| Elongation (5.65√S0 & 4D) | 16% | |
| Reduction of area | 50% | |
| Hardness (Brinell) | 277 min | |
| Impact strength (room temp) | 30 ft.lb | 41 J |
| Property | Imperial | Metric |
|---|---|---|
| 0.2% Proof stress (min) | 105.1 ksi | 725 N/mm² |
| Tensile strength (min) | 124.7 ksi | 860 N/mm² |
| Elongation (5.65√S0 & 4D) | 16% | |
| Reduction of area | 50% | |
| Hardness (Brinell) | 255 min | |
| Impact strength (room temp) | 55 ft.lb | 75 J |
| Property | Value |
|---|---|
| Density (kg/m³) | 7750 |
| Magnetic permeability (20°C) | < 1.1 |
| Young's modulus (kN/mm²) | 200 |
| Specific electrical resistance, 20°C (µΩ.m) | 0.8 |
| Mean coefficient of thermal expansion, 0-100°C (µ/m/°C) | 10.8 |
| Specific heat, 20°C (J/kg.K) | 460 |
| Thermal conductivity, 100°C (W/m.K) | 18.4 |
| Thermal conductivity, 500°C (W/m.K) | 22.7 |
Equivalents & cross-references
Standard designations
- UNS
- S17400The Unified Numbering System number for 17-4 PH.
- EN
- 1.4542The European material (Werkstoff) number for 17-4 PH. X5CrNiCuNb16-4The European chemical-composition designation for the same grade.
- AISI
- 630The AISI designation, also written Type 630.
- ASTM
- A564 Type 630ASTM A564 covers hot-rolled and cold-finished age-hardening stainless bar; Type 630 is 17-4 PH.
- ASME
- SA-564 Type 630ASME SA-564 Type 630 is the ASME adoption of ASTM A564 for pressure-retaining components.
- AMS
- 5643The aerospace material specification for 17-4 PH bar, wire, forgings and rings.
- NACE
- MR0175 / ISO 15156-3Sour-service materials standard; 17-4 PH is acceptable only in the double-aged H1150D condition, within its hardness limit.
17-4 PH is also designated UNS S17400, EN 1.4542, EN X5CrNiCuNb16-4, AISI 630, ASTM A564 Type 630, ASME SA-564 Type 630, AMS 5643 and NACE MR0175 / ISO 15156-3.
Common questions
What is the UNS number for 17-4 PH?
17-4 PH is UNS S17400, also designated EN 1.4542 (X5CrNiCuNb16-4), AISI 630 and ASTM A564 Type 630. It is a martensitic precipitation-hardening stainless steel.
What is 17-4 PH used for?
17-4 PH is used for aerospace components including landing gear and turbine blades; chemical processing pump shafts and valve components; food processing mixers and agitators; oil and gas components; surgical instruments; marine propeller shafts and fasteners; and pulp and paper industry components.
What are the conditions of 17-4 PH (Condition A, H900 to H1150D)?
Condition A is the solution-annealed starting condition, in which 17-4 PH is most readily machined and fabricated; it is then aged at a set temperature to reach the H conditions. H900 is aged at 482°C (900°F), H925 at 496°C, H1025 at 552°C, H1075 at 579°C, H1100 at 593°C and H1150 at 621°C, with H1150D double aged at 760°C then 621°C. The lower the ageing temperature the higher the strength and the lower the toughness: H900 gives a 0.2% proof stress of 1170 N/mm² (170 ksi), while H1150D gives 725 N/mm² (105.1 ksi) with the best toughness of the listed conditions, 75 J. We hold Condition A and H1150D from stock; the other tempers are aged to order.
What corrosion resistance and temperature limit does 17-4 PH offer?
17-4 PH offers corrosion resistance acceptable for many corrosive environments. Its high strength and toughness are retained at temperatures up to 316°C (600°F), supporting its use in oil and gas and chemical processing industries. It also has good resistance to wear.
What is AISI 630 stainless steel?
AISI 630 is the AISI designation for 17-4 PH, a precipitation-hardening martensitic stainless steel, also written Type 630. We stock it to ASTM A564 Type 630 and AMS 5643.
What is EN 1.4542 stainless steel?
EN 1.4542 (X5CrNiCuNb16-4) is the European designation for 17-4 PH, a precipitation-hardening martensitic stainless steel.
What is the density of 17-4 PH?
17-4 PH has a density of 7.75 g/cm³ (7750 kg/m³).
Is 17-4 PH magnetic?
Yes. 17-4 PH is a martensitic precipitation-hardening stainless steel and is magnetic.
How do you machine 17-4 PH?
17-4 PH machines best in Condition A (solution annealed), so where practical machine the part first and age it to the required H condition afterwards. Our datasheet gives Condition A turning speeds of 27 to 42 m/min (90 to 140 ft/min) for roughing and 35 to 60 m/min (120 to 190 ft/min) for finishing with carbide tooling, and 40 m/min (130 ft/min) for milling. Aged conditions are harder, so cut more slowly: about 69% of the Condition A speed for H900, rising to about the same speed as Condition A for H1150. Use enough coolant to prevent work hardening.
Can 17-4 PH be welded?
Yes, 17-4 PH can be welded using a compatible filler metal. Welding changes the heat-treated structure locally, so welded parts are usually heat treated again afterwards to restore their properties. The filler, any preheat and the post-weld treatment depend on the section size, the condition supplied and the service, so agree them with your welding engineer, and ask us which condition to buy for a welded fabrication.
How does 17-4 PH compare to 304 and 316 stainless steel?
17-4 PH has corrosion resistance comparable to Alloy 304 but is far stronger because it is precipitation hardened: in the H900 condition its 0.2% proof stress is 1170 N/mm² (170 ksi). Alloy 316L resists chloride pitting better because it contains molybdenum, but it is much lower in strength and cannot be hardened by heat treatment. 17-4 PH is martensitic and magnetic, whereas 304 and 316L are austenitic and essentially non-magnetic. Choose 316L where corrosion resistance matters most, and 17-4 PH where high strength, wear resistance and toughness are needed.
What certification is available for 17-4 PH?
EN 10204 3.1 material certificates are available for 17-4 PH on request, and additional documentation and certification can be supplied as required. Each bar is ultrasonically tested and visually inspected, and 17-4 PH bars are supplied peeled and polished to a surface finish of 125 CLA or better.
Is 17-4 PH suitable for sour service (NACE MR0175 / ISO 15156)?
Our 17-4 PH datasheet lists NACE MR0175 / ISO 15156-3 2015 among its specifications. 17-4 PH is acceptable for sour service under NACE MR0175 / ISO 15156-3 only in the double-aged H1150D condition, within its hardness limit; other conditions are not covered. State the condition and your service requirements when you enquire and we will confirm what we can supply.
Datasheets
17-4 PH bars are supplied peeled and polished to a surface finish of 125 CLA or better; each bar is ultrasonically tested and visually inspected.
Processing capability
Cutting
Automated band sawing to 650mm (25") section. CNC sawing at all sites.
Cutting servicesFirst-stage processing
Turning, boring and grinding undertaken in-house to help manage your supply chain.
Processing servicesInspection & testing
Each bar ultrasonically tested and visually inspected. Additional documentation and certification available.
Inspection & testingConditions & tempers
17-4 PH is supplied annealed (Condition A) for easy machining, then precipitation-hardened to the strength you need. Condition A and H1150D, the toughest aged condition, are held from stock; the other aged tempers, from H900 for maximum strength to H1150, are aged to order.
| Condition | 0.2% proof | Tensile | Hardness (HB) | Hardness (HRC) | Supply |
|---|---|---|---|---|---|
| Condition A | 380 N/mm² (55 ksi) | 1200 N/mm² (175 ksi) | 363 max | 39 max | From stock |
| H900 | 1170 N/mm² (170 ksi) | 1310 N/mm² (190 ksi) | 388 min | 42 min | Aged to order |
| H925 | 1070 N/mm² (155 ksi) | 1170 N/mm² (170 ksi) | 375 min | 40 min | Aged to order |
| H1025 | 1000 N/mm² (145 ksi) | 1070 N/mm² (155 ksi) | 331 min | 35 min | Aged to order |
| H1075 | 860 N/mm² (125 ksi) | 1000 N/mm² (145 ksi) | 311 min | 33 min | Aged to order |
| H1100 | 795 N/mm² (115 ksi) | 965 N/mm² (140 ksi) | 302 min | 32 min | Aged to order |
| H1150 | 725 N/mm² (105.1 ksi) | 930 N/mm² (134.8 ksi) | 277 min | 29 min | Aged to order |
| H1150D | 725 N/mm² (105.1 ksi) | 860 N/mm² (124.7 ksi) | 255 min | 25 min | From stock |
Aged tempers (H900 to H1150D) show guaranteed minimum properties; Condition A is the annealed state, shown at its maximum hardness. HRC figures are approximate conversions from Brinell (ASTM E140). Higher ageing temperatures trade strength for toughness and corrosion resistance. Full composition and the ageing cycle for each condition are in the 17-4 PH datasheet (PDF) (opens in new tab).
Request a quote
Tell us the grade, form and sizes.
Fast quotes from UK and US stock - bar, plate and pipe, cut and certified to spec.